UNS number | Composition | ||
---|---|---|---|
Pure zinc | Z13000 | 99.99 | 39.7 |
AC41A (Zamak 5) | Z35531 | Zn-4Al-1Cu-0.05Mg | 27.4 |
AC43A (Zamak 2) | Z35541 | Zn-4Al-2.5Cu-0.04Mg | 27.8 |
AG40A (Zamak 3) | Z33520 | Zn-4Al-0.04Mg | 27.4 |
AG40B (Zamak 7) | Z33523 | Zn-4Al-0.015Mg | 27.4 |
Copper-hardened rolled zinc | Z44330 | Zn-1.0Cu | 21.1 - 34.7 |
ILZRO 16 | Zn-1.25Cu-0.2Ti-0.15Cr | 27 | |
Korloy 2684 | Zn-22Al | 22 | |
Rolled zinc | Z21210 | Zn-0.08Pb | 32.5 |
Rolled zinc | Z21220 | Zn-0.06Pb-0.06Cd | 32.5 |
Rolled zinc | Z21540 | Zn-0.3Pb-0.03Cd | 39.9 |
Rolled zinc alloy | Z45330 | Zn-1.0Cu-0.01Mg | 21.1 - 34.8 |